Most of what we know about ageing comes from single cells on a bench, or from whole packs treated as a black box. Fischer and co-workers did something rarer: they took three field-aged Hyundai Kona Electric packs, measured each one intact, then measured every level again as they took it apart, from pack to module to parallel cell group to connector. We read the full paper, not just the abstract. This post is a companion to our pages on Remaining Useful Life, Cell to Cell Variation and State of Health, and it sits where those three meet.
Our verdict: treat this as a promising result from a small sample, not a settled rule. State of health came out similar for all three packs at roughly 95%. The more interesting finding is that a 1 ms, low-current resistance pulse added up from cells to pack to within 1.5%, while the 10 s DC pulse, the one we would normally use, did not (minus 2.4% to plus 6.9%, or minus 2.8% to plus 8.3% across the 1 s, 10 s and 30 s pulses). That is three packs of one model, so we cannot say the ordering would hold elsewhere, and the authors attribute part of the DC-pulse scatter to the voltage resolution of the pack-level equipment. Early-time ohmic resistance looks like a good candidate for a quality gate at end of line, in repair or in second-life grading, but it needs many more packs before we would call it the better tool. Capacity is the only one of the two metrics that found the limiting cell in this sample.
The paper: M. Fischer, M. J. Brand, A. Schröder and A. Jossen, “Teardown-Based cell-to-pack scaling of capacity and resistance in field-aged EV battery packs”, eTransportation 30 (2026) 100636, open access under CC BY 4.0 [1]. Numbers below are the authors’ unless we say they are our arithmetic.

What was tested
All three packs came out of Hyundai Kona Electric vehicles and use the same LG Chem E63B pouch cell: 63 Ah, 3.63 V nominal, 14.5 x 100 x 301 mm and 882 g [1]. From those figures we get about 229 Wh per cell and roughly 259 Wh/kg at cell level (our arithmetic, new-cell datasheet values). The packs were characterised 5 to 6 years after manufacture. The authors use “logical cell” for a parallel group, because a resistance or capacity measurement on a group cannot see differences between the cells inside it (see Cells in Parallel).
| Pack 1 | Pack 2 | Pack 3 | |
|---|---|---|---|
| Manufactured | 30 Jun 2020 | 26 Mar 2019 | 14 May 2019 |
| Nominal energy | 39 kWh | 64 kWh | 64 kWh |
| Nominal capacity / voltage | 126 Ah / 324 V | 189 Ah / 352.8 V | 189 Ah / 352.8 V |
| Topology | 90s2p | 98s3p | 98s3p |
| Modules | 6 sub-modules (15 logical cells each) | 10 sub-modules (eight of 10 logical cells, two of 9) | 10 sub-modules (eight of 10 logical cells, two of 9) |
| Module connectors + HVD | 8 + 1 | 12 + 1 | 12 + 1 |
| Logical cells | 90 | 98 | 98 |
Checking the series and parallel arithmetic. The topologies add up. Pack 1 is 6 modules of 15 logical cells, so 90 in series, and each logical cell is two 63 Ah cells in parallel (126 Ah, 180 cells). Packs 2 and 3 are 8 modules of 10 plus 2 modules of 9, so 98 in series, with three cells per logical cell (189 Ah, 294 cells). The paper’s “modules” are electrical sub-units. Our 2019 Hyundai Kona page, citing reporting on the vehicle, describes five physical modules in the 64 kWh pack: three under the floor with 20 series groups each and two stacked at the rear with 19 each. Splitting each of those into two sub-modules gives 6 x 10 + 2 x 10 + 2 x 9 = 98, which matches the paper (our reading). Two labelling points are worth knowing. First, the paper’s pack nominal voltages (324 V and 352.8 V) equal 3.6 V per logical cell, whereas its own cell table says 3.63 V, which gives 326.7 V and 355.7 V, the latter matching the roughly 356 V declared for the vehicle (our arithmetic). Second, the “nominal energy” of 39 and 64 kWh in Table 1 is not the product of nominal capacity and voltage: 126 Ah x 324 V is 40.8 kWh and 189 Ah x 352.8 V is 66.7 kWh (our arithmetic), so we read the paper’s figures as vehicle-level names, with 64 kWh being the usable energy of the 67.5 kWh gross pack on our Kona page. None of this affects the measurements, which are in ohms and amp-hours.
Only one vehicle model and one cell type are covered, and no field-use histories were available. The authors say plainly that the results are not population-wide estimates [1].
How it was measured
- Conditions: 25 °C, 50% SOC, with the packs rested for at least 24 hours before testing. Each level was measured before the next disassembly step.
- Capacity: logical cells only, by constant-current constant-voltage cycling at 0.4C with a C/50 termination between 2.5 V and 4.2 V. Our Cell Capacity Test Procedure page covers the general method.
- Early-time ohmic resistance (RΩ): a 1 ms low-current pulse (below about 0.05C) with the resistance evaluated at 400 µs, at pack, module, logical cell, connector and HVD level. The pulse method is covered by a patent cited in the paper (EP 3 438 682 B1) [1].
- DC-pulse resistance (RDC): a 30 s pulse at 0.4C, evaluated at 1 s, 10 s and 30 s, at pack and logical-cell level only. This is the familiar DCIR measurement.

The authors define capacity-based state of health per logical cell as:
where Cactual is the measured logical-cell capacity, CN the nominal capacity of one cell (63 Ah) and ncells the number of cells in parallel (2 or 3). Dispersion is the coefficient of variation (CoV), and they add a worst-case homogeneity indicator, SOHo, which compares the gap between the best and worst component with the best one [1].
Capacity: similar ageing, one pack more scattered
| Pack 1 | Pack 2 | Pack 3 | |
|---|---|---|---|
| Mean logical-cell capacity (Ah) | 120.35 | 179.11 | 179.83 |
| Spread, min to max (Ah) | 1.0 | 5.1 | 2.7 |
| CoV of capacity | 0.15% | 0.41% | 0.19% |
| Mean SOHC | 95.5% | 94.8% | 95.1% |
| Minimum-cell SOHC | 95.2% | 92.8% | 94.2% |
| Energy-based estimate for the minimum cell (SOHE) | 87.6% | 85.4% | 86.7% |
Pack capacity was not measured directly. The authors use the minimum logical-cell capacity as a proxy for what the pack would deliver in the 2.5 V to 4.2 V cell window (our post on Variability in Battery Pack Capacity covers how cell-to-cell spread sets pack capacity), and they note this is an upper bound on usable vehicle energy because the vehicle’s own voltage limits, balancing and thermal management will bite first [1]. To compare against Euro 7, which sets minimum battery energy retention of 80% at 5 years or 100,000 km and 72% at 8 years or 160,000 km [2], they convert capacity to energy using a literature ratio from Preger and co-workers [3]. All three packs sit above 85% on that basis. The authors are clear that this is context and not a compliance assessment, and we agree.
Resistance: cells dominate, connectors are not nothing
| Resistance (mΩ unless stated) | Pack 1 | Pack 2 | Pack 3 |
|---|---|---|---|
| 10 s DC-pulse resistance, pack | 81.98 | 68.91 | 65.10 |
| 10 s DC-pulse resistance, logical cell mean | 0.951 | 0.669 | 0.693 |
| CoV of logical-cell 10 s DC-pulse resistance | 2.07% | 3.80% | 2.40% |
| Early-time RΩ, pack | 51.19 | 40.83 | 40.00 |
| Early-time RΩ, module mean | 8.29 | 4.00 | 3.94 |
| Early-time RΩ, logical cell mean | 0.560 | 0.404 | 0.396 |
| CoV of logical-cell RΩ | 1.45% | 2.32% | 2.39% |
| Connectors + HVD, summed (RΩ) | 1.46 | 1.73 | 1.73 |
| Share of pack RΩ from connectors + HVD | 2.9% | 4.2% | 4.3% |
| 10 s DC-pulse pack resistance divided by pack RΩ (our arithmetic) | 1.60 | 1.69 | 1.63 |

Three things stand out. First, 10 s DC-pulse resistance, the figure we would normally quote and the one closest to the window a vehicle’s peak power is rated over, is about 1.6 to 1.7 times the early-time ohmic value at pack level (our arithmetic), which is the slower charge-transfer and diffusion contribution. Second, the logical-cell CoV of RΩ (1.45% to 2.39%) is several times the capacity CoV (0.15% to 0.41%), and the 10 s CoV (2.07% to 3.80%) is larger again, so resistance is the more sensitive indicator of heterogeneity in these packs. Third, the connectors and HVD add 1.5 to 1.7 mΩ, which is 3 to 4% of the pack’s ohmic resistance. The largest single items were a module connector at 567 µΩ and the HVD at 488 µΩ in Pack 1 [1].
Our arithmetic: take Pack 2 at 150 A (about 0.8C). The connectors and HVD at 1.73 mΩ drop 0.26 V and dissipate about 39 W (I2R), against roughly 6.1 V and 920 W for the whole 40.8 mΩ pack. This uses the 25 °C, 50% SOC, 1 ms ohmic value only, so real losses under load will be higher. It is a feel for scale, not a model, and it explains why interconnect design deserves attention even when the cells dominate. See Battery Pack Resistance for how the contributions build up.
Do the parts add up?
| Residual (calculated minus measured pack) | Pack 1 | Pack 2 | Pack 3 |
|---|---|---|---|
| RDC 10 s, from logical cells + connectors | +6.13% | -2.40% | +6.92% |
| RΩ, from logical cells + connectors | +1.35% | +1.25% | +1.42% |
| RΩ, from modules + connectors | 0.00% | +0.13% | +0.88% |
| RDC 1 s, from logical cells + connectors | +8.29% | -2.80% | +7.27% |
| RDC 30 s, from logical cells + connectors | +6.69% | -2.41% | +6.46% |

Taking the 10 s row first: the residuals are +6.1%, -2.4% and +6.9%, and they exceed the propagated uncertainty by factors of about 2.4, 1.0 and 3.0 (our arithmetic from Table 6 of [1]), so only Pack 2 sits at the uncertainty bound. The ohmic residuals are small and always positive. The authors’ explanation is that logical-cell measurements include tab welds and a short length of intercell busbar inside the voltage-sensing path, which the summed connectors do not account for: about 5 to 8 µΩ per logical cell [1]. The DC-pulse residuals are larger and change sign between packs. The authors attribute this to differences between the pack-level and cell-level measurement chains and to the stronger state dependence of a 10 to 30 s pulse. Our reading is that the longer pulses are measuring more physics (diffusion, charge transfer) and more of the test equipment at the same time, so they close less cleanly. They also report that at logical-cell level the DC-pulse dispersion cannot be separated from measurement uncertainty on a conservative criterion, whereas the ohmic dispersion can [1].
Does a weak cell show up as a resistive cell?
Not reliably. The correlation between logical-cell capacity and RΩ was weakly negative in Packs 1 and 3 (r = -0.21 and -0.13, neither significant at the 5% level) and moderately positive in Pack 2 (r = 0.44) [1]. Our reading, which the authors also suggest, is that a parallel group’s resistance is dominated by its healthiest branch, so one weak cell inside a group can hide. Capacity found the limiting group in each pack; resistance did not. That is a useful reminder for any SOH algorithm that leans on resistance alone.
One small positional effect is worth knowing about: the last logical cell in a module consistently read lower in resistance, and the authors link this to the connection geometry, with the two connector types differing by about 22 µΩ [1].
Caveats
- Three packs, one vehicle, one cell type, no field histories. Treat the numbers as a case study, not as population data [1].
- Capacity is measured at logical-cell level after teardown. Pack capacity is inferred from the minimum cell and is an upper bound on vehicle-usable energy [1].
- Resistance is measured at 25 °C and 50% SOC only. Nothing here says how the ranking behaves at low temperature or high SOC.
- The 1 ms pulse method is the authors’ own patented approach, and the measurement devices were supplied by Li.plus GmbH, an affiliation declared in the paper (one author reports equipment supplied by the company, and another lists it as an affiliation) [1]. We have no reason to doubt the data, but the method has not been compared here with other early-time techniques.
- The data are available on request only [1], so we cannot re-use the cell-by-cell values directly.
What to take from this
For the BMS and diagnostics team: on this sample, capacity and early-time ohmic resistance are complementary, not interchangeable. Use capacity to find the limiting group and ohmic resistance to check the hardware around it. For manufacturing and repair: a simple series sum of the measured components reproduced the pack ohmic resistance to within 1.5% for these three packs, which suggests resistance could be a workable check at each assembly step, as the authors propose [1]. For second-life grading, the 3 to 4% connector contribution is a fixed overhead that does not age with the cells, so it should be separated before blaming the cells for a rise in pack resistance. The authors are careful that pass and fail thresholds would need reference distributions from many more packs, and we would add that to this list [1]. For the broader ageing picture see Remaining Useful Life and Performance Imbalances in Parallel-Connected Cells.
Nigel: Typically we assume an additional 10 mΩ for pack resistance on top of that given by the cells. That rule of thumb is much larger than what this paper measured: the connectors and HVD come to 1.5 to 1.7 mΩ, and the gap between the summed logical cells and the measured pack is under 1 mΩ.
Nigel: Typically we would use 10 s resistance data. Either way, this is a big conclusion to draw from one set of data, and we would need many more packs and values to state it fully. 10 s resistance also lines up with the cell values we usually quote and with the vehicle’s maximum peak performance.
Module count: our 2019 Hyundai Kona page says five modules. The reporting it relies on gives three floor modules with 20 series groups each and two rear modules with 19 each. Splitting each into two sub-modules gives 6 x 10 + 2 x 10 + 2 x 9 = 98, exactly the paper’s layout. The paper’s “modules” are the sub-units, so there is no conflict.
Bottom line: after 5 to 6 years the cells in these three Kona packs had aged similarly (about 95% SOH). In this small sample a 1 ms ohmic pulse explained the pack resistance to within 1.5% and put 3 to 4% of it in the connectors and HVD, and only capacity could point to the limiting cell. Three packs from one model is not enough to generalise from.
References
- M. Fischer, M. J. Brand, A. Schröder, A. Jossen, “Teardown-Based cell-to-pack scaling of capacity and resistance in field-aged EV battery packs”, eTransportation 30 (2026) 100636. doi:10.1016/j.etran.2026.100636
- Regulation (EU) 2024/1257 of the European Parliament and of the Council of 24 April 2024 (Euro 7), as cited in [1]. EUR-Lex
- Y. Preger, R. Wittman, S. Harris, M. Dubarry, “Are capacity and energy loss equivalent metrics for battery aging reporting?”, J. Electrochem. Energy Convers. Storage 2026; 23(2):021109, as cited in [1]. doi:10.1115/1.4071224
See also: Lifetime, Electrochemical Impedance Spectroscopy, Four-Wire (Kelvin) Resistance Measurement
Get the next teardown in your inbox
New teardowns, benchmarks and design data from BatteryDesign.net, free by email. Unsubscribe any time.