Commercial pouch cells stop growing at about 15 mm thick, and the reason is not one limit but four that arrive at roughly the same place. Our Pouch Cells page states the ~15 mm figure in a single line. This post shows where it comes from, using the 375 pouch cells in the BatteryDesign.net Cell Database that have all three dimensions populated.
The median pouch cell is 9.0 mm thick. Only 13 of the 375 are thicker than 15 mm, and the thickest is a 24.3 mm BYD LFP cell, which we come back to at the end. The distribution also has two humps, one near 6 mm and one near 10.5 mm; our reading is that this separates consumer and power-tool cells from automotive cells, but we have not yet split the data by application to prove it.

The thin end: packaging overhead
The minimum is set by the packaging, which does not shrink with the cell. The laminate walls, sealant layers, seal flange and tab sealant are much the same on a 2 mm cell as on a 12 mm one, so the thinner the cell, the larger the share of it that stores no energy.
One consumer-electronics patent puts a number on it: a 1.5 mm cell with a 91 µm pouch spends 12.1% of its thickness on packaging, and the patent’s aim is to cut that to 7.3% with a thinner film [1]. That is why the smallest cells in the database sit around 1.5 to 2 mm, in phones, tablets and wearables, where the device thickness forces the issue.
Below that are the single-layer and two-layer pouches built by research groups. Their job is to test a chemistry in a realistic mechanical environment, not to sell energy. Bridgewater et al. ran identical coatings in coin cells, single-layer pouches and stacked pouches and found the trends carried across all three formats, but true energy and power density still only come from a properly engineered stacked or wound cell [2]. A one-layer pouch is a test fixture, not a product.
Limit 1: how deep the laminate will draw
The pouch is not folded around the stack; a cup is pressed into the aluminium-laminated film with a punch and die, and the stack sits in that cup. The aluminium layer only stretches so far before it thins, cracks or pinholes, and it fails first at the punch corners where the strain is highest. Our Pouch Cell Edge Seal Integrity page covers the laminate and why its foil is specified for elongation.
The patent literature is consistent on the numbers:
- Common laminates draw to about 6 to 8 mm before the aluminium tears [3].
- Drawing both halves and sandwiching the stack between them gives a finished cell of about 12 to 16 mm [4].
- Better laminates with a ~10 mm draw stretch that to 10 to 20 mm [5].
So the ~15 mm ceiling on our Pouch Cells page is a forming limit first. Going deeper on a single draw means a better foil, slower forming, more scrap, or a different way of making the housing.
Limit 2: how many foils one weld will take
Every cathode foil in the stack is gathered and welded to one aluminium tab, and every anode foil to one nickel or nickel-plated copper tab, usually by ultrasonic welding. The more layers, the more energy the weld needs to reach the bottom foil, and the more the top foils get marked, cracked or shed as particles.
Weld equipment suppliers put the reliable limit at 40 to 50 foil layers per tab [6], with damage and particulates rising as counts approach or pass 60 [7]. Laser welding and two-step joints (foils first, then the tab) are the industry’s ways round it.
A quick estimate shows why this lines up with the forming limit. Taking a typical automotive repeat unit (our assumed values, not a specific cell):
| Layer | Thickness (µm) |
|---|---|
| Double-sided cathode on 15 µm Al | 130 |
| Double-sided anode on 8 µm Cu | 150 |
| Two separators | 24 |
| Repeat unit | ~300 |
A 15 mm stack carries about 50 cathode foils on one tab: right at the welding limit. Thicker, higher-loaded electrodes need fewer foils for the same thickness, which is one way a cell can go thicker without breaking the weld, at the cost of rate capability.
Limit 3: getting the heat out
A stack of electrodes is a poor conductor through its thickness and a good one along its foils. Lin et al. measured a 20 Ah LFP pouch at about 0.51 W/m·K through-plane against about 26.5 W/m·K in-plane, a ratio of around 50 [8]. Our Thermal Management hub explains the anisotropy.
For a face-cooled cell with uniform heat generation, the centre-to-surface temperature rise is:
where q̇ is the volumetric heat generation (W/m³), k the through-plane conductivity (W/m·K), and L the conduction path: half the cell thickness when both faces are cooled, the full thickness when only one is.
The point is the square. Using q̇ = 50 kW/m³ and k = 0.5 W/m·K (our assumed values, roughly a hard fast charge):
| Cell thickness (mm) | ΔT, both faces cooled (K) | ΔT, one face cooled (K) |
|---|---|---|
| 9 | 1.0 | 4.1 |
| 15 | 2.8 | 11.3 |
| 24 | 7.2 | 28.8 |
That gradient matters beyond peak temperature. Cloos and Wetzel found that a through-plane gradient accelerates capacity loss more than an in-plane gradient of similar size [9], so the inner layers of a thick cell age differently from the outer ones.
This is also why automotive pouch modules settled on edge cooling, as our Pouch Cell Cooling and Pouch Cell Design and Edge Cooling posts show: it uses the in-plane path. Edge cooling relaxes the thickness penalty but does not remove it, because a thicker cell puts more heat through the same edge length.
Limit 4: wetting, formation and swelling
The last two limits are softer, but they push the same way.
Wetting. Electrolyte reaches the pores by capillary action, and every extra layer and every extra micron of coating slows it down. TUM’s work on large-format cells notes that more layers, thicker electrodes and more area per cell all lengthen wetting, and that industrial filling, wetting and formation together take 1.5 to 3 weeks [10]. A thicker cell spends longer on the most expensive floor space in the plant, and a stack that is not fully wetted risks local plating at formation.
Swelling. Electrodes breathe with state of charge and the stack grows with age and gas. One pouch-frame patent cites swelling of up to 8 to 10% over 500 cycles for some pouch cells [11]; that is a patent’s background claim, not a test report, but even half that figure on a 24 mm cell is over a millimetre the module must absorb. See our Cell Electrode Pressure post for why that growth has to be held at a controlled pressure.
Where the limits land
| Limit | Where it bites | Hard or soft | Way round it |
|---|---|---|---|
| Packaging overhead | Below ~2 mm | Soft (cost and Wh/L) | Thinner laminate |
| Laminate draw depth | ~12 to 16 mm (two halves drawn) | Hard | Better foil, folded or welded housing |
| Foil-to-tab weld | ~15 mm (40 to 60 foils) | Hard | Thicker electrodes, laser or two-step welds |
| Through-plane heat | Grows with thickness squared | Depends on duty | Edge or tab cooling, lower C-rate |
| Wetting and formation | Grows with layers | Soft (cycle time) | Vacuum filling, ceramic separators |
| Swelling | Grows with thickness | Soft (module design) | Compression, foam, space allowance |
Two of these are hard manufacturing limits and both land at about 15 mm. The thermal limit sits close behind for any cell that is fast charged or face cooled. That is why 362 of our 375 pouch cells are 15 mm or thinner: going further means changing the housing process, the electrode design and the duty cycle all at once. For a traction cell, that trade rarely pays.

The outlier: BYD CB98 at 24.3 mm
The thickest pouch cell in the database is BYD’s CB98, and it shows that 15 mm is an economic limit for traction cells, not a law of physics. Its manufacturer specification, as held in the Cell Database [12]:
| Parameter | Value |
|---|---|
| Chemistry | LFP |
| Dimensions (mm) | 257.5 (incl. tabs) × 91.3 × 24.3 |
| Capacity / energy | 47.7 Ah / 152.6 Wh |
| Mass (kg) | 1.01 |
| DCIR (mΩ) | 1.2 to 1.8 |
| Continuous charge / discharge (A) | 50 / 120 |
| 10 s peak charge / discharge (W) | 500 / 950 |
Our arithmetic gives about 151 Wh/kg and about 267 Wh/L, the volume including the tabs.
The specification says what the cell is for. Its discharge temperature range carries a note that operation from -35 to -30 °C is for BSG (belt starter-generator) starting only. Our reading is that this is a low-voltage start and mild-hybrid cell: four in series make a 12.8 V battery that drops into a lead-acid footprint, where the box sets length and height and thickness is free.
That duty cycle also forgives the limits above:
- Heat. Continuous ratings are about 1C charge and 2.5C discharge, and the high-power events last seconds. An auxiliary battery spends most of its life near idle, so the thickness-squared penalty rarely gets a chance to bite.
- Forming. At 91 mm tall, the cup is small in plan, which is a different forming problem from a 100 × 300 mm traction pouch. Whether BYD uses a very deep double draw or a folded housing is not published.
- Welding. On our 0.3 mm repeat unit, 24 mm would mean about 80 foils per tab, well past the 40 to 60 range. Thicker LFP coatings or two sub-stacks welded separately would explain it, but we could not find a teardown that confirms either.
Change the application and the limit moves. For a fast-charged traction cell, 15 mm is still where the trade stops paying.
References
- US 9,812,677: Reducing pouch thicknesses in battery cells for portable electronic devices
- Bridgewater, G. et al., A Comparison of Lithium-Ion Cell Performance across Three Different Cell Formats, Batteries 2021, 7(2), 38
- US 10,992,005: Deep pouch cell and method of manufacturing same
- US 11,050,103: Pouch cell and method of forming same
- US 11,424,501: Deep format pouch for battery cell
- Battery Technology, Need More Reliable Metal Bonds? This Ultrasonic Welding Innovation Is a Key, August 2021
- Machine Design, Foiling Damage to Thin-Metal Welding
- Lin, J., Chu, H.N., Monroe, C.W., Howey, D.A., Anisotropic thermal characterisation of large-format lithium-ion pouch cells, arXiv:2112.09768
- Cloos, L. and Wetzel, T., In-Plane versus Through-Plane Thermal Gradients during Cyclic Aging of Lithium-Ion Batteries: An Experimental Study, KIT
- TUM iwb, electrolyte filling and wetting of large-format cells (mediaTUM 1525531)
- US 11,158,897: Multifunctional pouch battery cell frame
- BatteryDesign.net Cell Database v1.8.24, entry for BYD CB98 47.7 Ah (from manufacturer specification)
See also: Pouch Cells, Pouch Cell Edge Seal Integrity, Pouch Cell Cooling, Pouch Cell Design and Edge Cooling, Cell Electrode Pressure, Golden Ratio for Cell Design, Battery Thermal Management, Cell Formats
Get the next teardown in your inbox