Self-discharge is the slow loss of a cell’s stored charge while it sits with no load connected. It comes from small parasitic side reactions inside the cell, and from any leakage path through the electrolyte, separator or contamination. A fault such as a micro short makes it worse. The rate matters for shelf life, for how long a pack can be stored before it needs a top-up, and in production as a screen for faulty cells. This page describes how it is measured; the pack-level equivalent, which includes the BMS and other electronics, is the Stand Test.
What is being measured
There are two quantities that are easy to confuse. Reversible self-discharge is charge that is lost but can be recovered, for example by charge redistribution inside the electrodes. Irreversible self-discharge is charge consumed by side reactions such as continued SEI growth, which permanently reduces the lithium available. A good procedure separates these by measuring capacity before and after the storage period.
Test methods
- Capacity loss method. Measure capacity with the Cell Capacity Test Procedure, recharge to the specified state of charge, store the cell open circuit at a controlled temperature, then discharge it again and compare. It is the most direct and reflects the real loss, but needs full cycles either side of the rest period.
- Voltage decay method. Charge to a set state of charge, rest, and log the open circuit voltage over days to weeks. The voltage drop is converted to a charge loss using the cell’s OCV-SoC curve. It is simple, but the conversion is weak on chemistries with a flat OCV curve, such as LFP.
- Voltage hold (potentiostatic) method. Hold the cell at a fixed voltage with a very stable, high-resolution supply and measure the small current needed to keep it there. That current approximates the self-discharge current, and the result settles far faster than waiting for the voltage to fall. Equipment vendors describe this as a way to cut a measurement from weeks or months to a much shorter time (see the Keysight application note)
Procedure outline (capacity loss method)
- Bring the cell to the test temperature and confirm it has stabilised; self-discharge roughly increases with temperature, so keep it controlled and recorded.
- Run a reference capacity measurement and record the discharged capacity.
- Charge to the target state of charge (commonly full, but a mid-SoC test is useful for storage studies) and allow a relaxation rest.
- Disconnect all loads and store open circuit for the defined period, logging voltage and temperature at intervals.
- Discharge at the reference rate and record capacity. Self-discharge is the difference from the pre-storage capacity, usually expressed as a percentage per month.
- Optionally run a further full cycle to find how much of the loss was recoverable.
Why the first weeks are misleading
A freshly formed cell is still settling. Work by Roth and colleagues at TU Munich compared voltage decay, voltage hold and capacity loss methods and reported that early transients die away within hours, whereas the slow redistribution of lithium across the anode overhang area went on skewing every electrical method for a matter of weeks (see Relaxation Effects in Self-Discharge Measurements of Lithium-Ion Batteries, Journal of the Electrochemical Society, 2023). They also noted that voltage-based methods under-represent this effect. In practice a self-discharge figure taken soon after formation can overstate the real rate, and a production screen needs a rest long enough to get past it.
Common sources of error
- Insufficient relaxation before the first voltage reading, so the decay is dominated by polarisation recovery rather than self-discharge.
- Temperature drift, which changes both the rate and the voltage reading.
- Voltmeter input current and fixture leakage, which are comparable to the signal on a very low-leakage cell.
- Using a flat OCV region (typical of LFP) to infer charge loss from voltage.
- Comparing cells at different states of charge, since the rate varies with SoC.
Where the result is used
- Production screening: an outlier with high self-discharge is a candidate for an internal short. See End-of-Line (EOL) Cell Production Testing.
- Storage and shelf-life estimates, and the allowable time between top-up charges.
- Cell matching for series strings, where mismatch in self-discharge drives imbalance over time.
- Separating cell leakage from BMS and electronics draw in a pack.
References
- Roth, Streck, Graule, Niehoff, Jossen. Relaxation Effects in Self-Discharge Measurements of Lithium-Ion Batteries. J. Electrochem. Soc. 170(2), 2023
- Keysight. Evaluate Self-Discharge of Lithium-Ion Cells in a Fraction of the Time Traditionally Required (application note)
See also: Stand Test, Cell Capacity Test Procedure, HPPC Test Procedure, Cell Testing, Key Cell Metrics, Self Discharge of Cells, Remaining Capacity, Cell Internal Short Circuits, Cell Internal Short Circuit Device, Relaxation delta Voltage