A team from Imperial College London, UCL and the Faraday Institution has shown that, for lab-made NMC811 cathodes, measurements taken before calendering can predict thickness and early-cycle capacity after it. The test-set fits are good (R² of 0.77 for thickness and 0.93 for capacity), but the way the data was split means those numbers are a best case. The idea is worth more than the headline accuracy.

Zhen Zhao, Chu Lun Alex Leung, Chun Huang, Machine learning enabled cross-stage prediction of cathode performance using manufacturing parameters and measured electrode descriptors, Journal of Energy Storage, Volume 182, Part C, 2026
Most machine-learning work on electrode manufacturing maps process settings straight to an electrode property, or straight to cell performance. This paper asks a question closer to what a line engineer actually faces: I have already measured this web upstream, so what will it look like once it has been through the calender, and how will the cell perform?
What they made and measured
Every data point is a real measurement: 160 electrode discs and 99 coin cells, with no simulated data. Each coated sheet was split. Discs punched before calendering form Group A; discs punched from the same sheet after calendering form Group B. Pairing A with B within a batch is what makes the cross-stage models possible.
| Item | Value |
|---|---|
| Active material | NMC811, with C65 carbon black and PVDF in NMP |
| Formulation range (wt%) | NMC811 84–96, C65 2–8, PVDF 2–10 |
| Solid-to-liquid ratio | 75–135% (by mass) |
| Coating | Doctor blade, 300 µm wet gap, 15 mm/s, on Al foil |
| Drying | 48 h in a fume hood, then 2 h vacuum at 80 °C |
| Calendering | Single pass, unheated rolls, 0.1 cm/s, gap set on the dial at 50–100 µm |
| Group A (uncalendered) | 104.0 ± 11.8 µm, 10.6 ± 2.3 mg/cm² active, 183.4 mAh/g mean |
| Group B (calendered) | 74.2 ± 9.0 µm, 11.5 ± 2.8 mg/cm² active, 206.4 mAh/g mean |
| Cells | CR2032 half cells vs Li metal, Celgard 2400, 70 µL 1 M LiPF₆ in EC/EMC 1:1 |
| Test | 0.1C, 2.8–4.3 V, five cycles only |
Two details are worth noting. The formulation and the solid-to-liquid ratio were not varied independently: richer binder and carbon mixes were made wetter to keep them coatable. And the within-batch spread is large. The authors’ variance decomposition puts disc-to-disc variation at 24.5–32.0% of total variance before calendering and 14.4–19.3% after.
The eight models
Six first-stage models predict a property from process settings plus measured disc mass or thickness. Two cross-stage models predict a calendered property from its uncalendered twin. All eight use gradient boosting regression (GBR), chosen after a comparison with random forest, support-vector regression and a neural network. The neural network did badly on datasets this small, which is no surprise.
| Model | Inputs | Predicts | Test records | Test R² | NRMSE |
|---|---|---|---|---|---|
| Mass loading, before calender | Formulation, S/L ratio, thickness | Active mass loading | 15 | 0.94 | 3.8% |
| Mass loading, after calender | As above + calender gap | Active mass loading | 15 | 0.36 | 8.78% |
| Thickness, before calender | Formulation, S/L ratio, electrode mass | Thickness | 16 | 0.89 | 4.75% |
| Thickness, after calender | As above + calender gap | Thickness | 16 | 0.93 | 3.18% |
| Capacity, uncalendered cells | Formulation, S/L ratio, mass, thickness, cycle number | Specific capacity, cycles 1–5 | 39 | 0.93 | 5.41% |
| Capacity, calendered cells | As above + calender gap | Specific capacity, cycles 1–5 | 51 | 0.93 | 4.36% |
| T2T | Thickness A, mass ratio A/B, calender gap | Thickness B | 30 | 0.77 | 5.26% |
| C2C | Capacity A, mass ratio A/B, calender gap, cycle number | Capacity B, cycles 1–5 | 64 | 0.93 | 2.21% |
S/L = solid-to-liquid ratio of the slurry. NRMSE = root-mean-square error normalised to the range of the target. Test records are cycle-level for the capacity models, so one cell contributes up to five.
What the results say physically
Strip away the algorithm and most of the findings are ones a process engineer would expect. That is reassuring: the models are learning physics, not noise.

T2T model dataset and prediction results. a, 3D distribution of the cleaned T2T dataset (n = 149 within-batch A–B electrode combinations): the axes show the thickness (A), the electrode mass ratio, and the calendering gap, and the point colour indicates the measured Group B thickness. b, Predicted and measured Group B thickness for the held-out test set (n = 30 combinations): blue diamonds denote measured values and orange circles denote predicted values. c, Parity plot for the test set: the black solid line is the y = x reference and the point colour indicates the local density of the data points. d, Test-set residuals: the solid blue line shows the smoothed residuals (residual = measured − predicted) and the orange dashed line marks zero error. e, GBR feature importance scores; bar height denotes feature importance, and bar colour carries no additional information. MR: electrode mass ratio (mass (A) / mass (B)); T(A): thickness (A); CG: calendering gap. Held-out test-set performance (R2/MSE/NRMSE) was 0.77/15.06/5.26%.
Calendering does not change loading, so the gap cannot predict it. Pressing a coating changes its thickness and porosity, not the mass of active material per square centimetre. The post-calender mass loading model was the weakest in the set (R² 0.36), and the SHAP analysis ranked the calender gap as its least useful input. Note that Group B’s mean loading (11.5 mg/cm²) sits above Group A’s (10.6 mg/cm²), even though the discs came from the same sheets. The calender cannot add mass, so that difference is disc-to-disc coating variation, and it is as big as many of the effects being modelled.
Before the calender, thickness follows mass; after it, thickness follows the gap. The ablation study shows this clearly. With measured electrode mass alone, uncalendered thickness is predicted with R² 0.89; with the process settings alone, the model is no better than the mean (R² −0.03). After calendering it flips: process settings alone give R² 0.88, because the roll gap now sets the answer.
Springback matters. In the thickness-to-thickness (T2T) model, the gap, the A/B mass ratio and the pre-calender thickness carried similar weight (importance 0.39, 0.37 and 0.25). If the electrode simply ended up at the set gap, the gap would dominate. It doesn’t, because porous coatings recover elastically after the nip and also compact unevenly. See our Calendering page for the mechanics.
At C/10, capacity is mostly about conductive carbon. C65 content was the top feature in both capacity models, and it correlated positively with specific capacity (0.55 uncalendered, 0.26 calendered). Calendered cells averaged 206.4 mAh/g against 183.4 mAh/g uncalendered. The likely reading is that loose, uncalendered films have a patchy electronic network, and both more carbon and compaction fix it. For uncalendered cells, formulation dominates so strongly that a model using only process settings (plus cycle number) matched the full model (R² 0.95 versus 0.93). For calendered cells, process settings alone dropped to R² 0.75, so measured mass and thickness add real information once the film has been pressed.
Before you lean on the numbers
The authors call this a preliminary lab-scale proof of concept, and they are candid about its limits. Five points matter most if you are thinking of applying it.
- The train/test split leaks. Records were split at random, not by batch or by cell. Discs from the same batch, and cycles from the same cell, can sit on both sides of the split. In the capacity models, five cycles per cell means the model can often see the same cell’s neighbouring cycles while training. That inflates test R². A grouped split, holding out whole batches, is the test that would tell you how the method handles a new formulation. The authors flag this themselves.
- The test sets are small. The first-stage models were scored on 15–16 discs. On sets that small, R² swings a lot with the random seed. The post-calender loading model, for example, scored −0.16 with default settings and 0.36 after tuning, and a support-vector model beat both at 0.58.
- Outliers were removed before the split. Isolation Forest screening dropped up to 7% of records from each full dataset, test records included. That is common practice, but it means the test set has been cleaned in a way live production data would not be.
- “No post-calendering measurements” needs a footnote. The cross-stage models use the mass ratio of the paired A and B discs, and the B disc was weighed after it had been calendered. Mass does not change in the calender, so on a real line the equivalent number could come from an upstream areal-weight gauge tracked to the same web position. The concept holds, but it relies on that tracking.
- The domain is narrow. The electrodes were lab-coated and dried slowly in air, and calendered by gap setting rather than line load. Areal capacities work out at roughly 1.9–2.4 mAh/cm² (loading × measured capacity), well below typical automotive cathodes; see Areal Loading. Testing stopped at five cycles at C/10 in half cells, so rate capability and porosity-limited transport, where calendering matters most, were not tested. Porosity and density were not reported. The data is available on request only.
None of this undermines the paper. It just means the R² values describe interpolation within one lab’s dataset, not a validated predictor for a new line.
Why it matters on a production line
The useful idea is the structure, not the accuracy figures. A coating line already measures areal weight and wet or dry thickness before the calender. If those readings, plus the formulation and the planned roll setting, can predict post-calender thickness, the calender can be set feed-forward instead of corrected after the fact. Predicting early capacity from the same upstream data points at catching a bad roll before it is slit, stacked and formed.
The T2T result is the part to watch. It says the gap setting alone is not enough to hit a target thickness: the incoming coating’s own thickness and mass carry nearly as much information. Anyone who has chased springback on a calender will recognise that.
To be usable on a line, the next step is the one the authors list: pilot-line data, calendering defined by line load and roll temperature rather than a dial, and validation that holds out whole batches. Until then, treat the paper as a well-documented template for how to structure the problem.
Bottom line: a sensible, honestly reported lab study. The physics it recovers is sound and the cross-stage framing is the right one. The headline R² values are optimistic because of how the data was split, so they should not be quoted as what to expect in production.
Reference
- Z. Zhao, C.L.A. Leung, C. Huang, “Machine learning enabled cross-stage prediction of cathode performance using manufacturing parameters and measured electrode descriptors”, Journal of Energy Storage 182 (2026) 124825. doi.org/10.1016/j.est.2026.124825. Open access, CC BY 4.0.
See also: Calendering, Importance of Electrode Parameter Changes After Calendaring, Hot versus Cold Roll Calendering, Coating, Drying, Areal Loading, Cathode Testing and Validation
Get the next teardown in your inbox
New teardowns, benchmarks and design data from BatteryDesign.net, free by email. Unsubscribe any time.