The impact of state of charge on transport in silicon anodes

Quantifying microstructure differences across Gr-SiOx anodes stopped at states of charge from 0 to 100%.

Introduction

Fast charging in graphite-silicon suboxide (Gr-SiOx) composite anodes depends on maintaining efficient ionic transport as the electrode evolves during lithiation. This is particularly challenging because the two active phases undergo different degrees of dimensional change. SiOx offers substantially higher specific capacity than graphite, but also expands much more strongly during lithiation. Graphite expands to a lesser extent, while the surrounding pore network must accommodate the combined volume changes without losing the connected pathways required for lithium-ion transport.

This creates a coupled microstructural problem. As the active phases expand, pore space can be consumed, the electrode can increase in thickness, and the remaining pore pathways can become more tortuous. Measuring any one of these effects in isolation therefore provides only a partial picture. Pore fraction, for example, indicates how much void space remains, but not whether that space still forms an efficient through-plane transport network.

The central question in this study is therefore: where is lithiation-associated dimensional change accommodated within a Gr-SiOx anode, and what does that imply for transport through its pore network?

To investigate this question, we combined quantitative cross-sectional scanning electron microscope (SEM) analysis with generative 3D reconstruction. The 2D segmentations were used to measure porosity fraction, electrode thickness and SiOx particle size. Reconstructed 3D volumes were then used to calculate pore-network tortuosity. Together, these measurements connect changes at the particle, electrode, and transport-pathway scales.

From multi-detector SEM images to linked microstructural measurements

Fifteen cells (NMC811 cathode, Gr-SiOx anode) were assembled and, after formation, were charged to one of five SoCs: 0, 25, 50, 75 and 100%. This gave three electrode samples at each SoC to improve the reliability of the results. N.B. The 0% group represents electrodes that were charged and then returned to a delithiated state rather than pristine, uncycled electrodes. 

The 15 electrode samples were harvested from their cells during teardown in an inert-atmosphere glovebox. They were then prepared for SEM imaging as cross-sections using broad-beam ion milling (BBIM). An air-protected transfer system was used to minimise exposure to the ambient atmosphere. As different electrodes were examined at each SoC (rather than following the same electrode through charge), it is not possible to track the same particles, so it’s important to collect statistically representative data in order to draw valid conclusions. 

Each SEM image was acquired using three detectors simultaneously: backscattered, secondary, and in-lens. Figure 1 displays a section of the image containing the signal from each of these detectors. The signals were stacked using Polaron so that compositional and morphological information could be used together to generate features during segmentation.

Figure 1: Merged images of a sample anode in Polaron used to extract information from various detectors (from left to right: BSE, SE and Inlens). The scale bar is 30 μm.

The electrode coating was segmented into three phases: SiOx, graphite and pore, in addition to identifying the current collector and the material above the electrode (i.e. the background).

The analysis was structured around four related questions:

  • Phase fractions: How does the internal porosity change with SoC, and which phases balance out this change?
  • Electrode thickness: Does the expansion of the particles change the electrode thickness?
  • SiOx particle size: How does lithiation-associated expansion of SiOx appear in particle size measurements across SoCs?
  • Pore tortuosity: How do changes in the remaining pore network affect the predicted transport resistance?
Figure 2: Polaron workflow, from SEM image to segmentation to 3D reconstruction on a 25% SoC anode.

Image-based analysis is valuable because the measurements remain visually auditable. Ion milling is destructive, so acquiring an exact replacement section may not always be possible; nevertheless, the images provide strong local evidence of what produced an unusual result. This complements bulk and spectroscopic techniques such as X-ray diffraction or impedance, whose signals are more difficult to assign to a specific local microstructural feature. Figure 2 displays a representation of the workflow from raw SEM image to segmentation, to three-dimensional volume using Polarons reconstruction module.

Phase fractions show that pore loss is the first large structural difference

The phase fractions extracted from the segmented image data are reported in Figure 3. The error bars represent the standard deviation across the independently prepared electrodes at each SoC and thus capture electrode-to-electrode variability. The mean segmented pore fraction decreases from approximately 0.37 at 0% SoC to 0.19 at 50% SoC, then remains between 0.17 and 0.19 through to 100%. The largest change in porosity therefore occurs in the first half of the sampled SoC range. The graphite fraction increases over the same interval, while the mean SiOₓ fraction remains approximately stable through 75% SoC and is higher in the 100% group. One sample at 25% SoC showed substantial delamination and was excluded from the phase fraction comparison.

Figure 3: Mean segmented phase fractions vs state of charge (SoC)
Figure 4: Polaron segmentation enables the out-of-plane sections (Blue) and current collector (Orange) to be segmented out, only calculating the expansion region (Green).

The thickness of the electrodes was also measured from the images as the mean vertical distance from the separator to the top surface (as displayed in Figure 4) and reported in Figure 5. The thickness remains approximately constant from 0% to 75% SoC, with group means of 56.1, 57.1, 55.3 and 56.6 µm, respectively. At 100% SoC, the mean increases to 63.1 µm. All sections in the 100% group have greater measured thicknesses than the sections at lower states of charge.

Taken together, the two measurements suggest a possible two-scale accommodation mechanism. The lower-SoC groups are associated with a large reduction in pore fraction without a corresponding increase in coating thickness, whereas the 100% group combines a thicker coating with little further change in relative pore content. One interpretation is that dimensional change is initially accommodated within the pore space and becomes more apparent at the coating scale once that internal accommodation is reduced.

Figure 5: Electrode thickness as a function of SoC.

Larger SiOx particles accompany the thicker 100% SoC coating

The segmented SiOx particle sizes were measured using Feret diameter; particles below 0.4 μm were excluded to remove noise. The distribution was then weighted by area, and from that the D10, D50 and D90 were calculated and are displayed in Figure 6.

Figure 6: Area-weighted SiOx particle sizes D10, D50 and D90 versus state of charge.

SiOx particle size changes only slightly between 0% and 75% state of charge. At 100%, the particles are larger. The average D50 size rises from 4.9 μm to 5.7 μm, about a 16% increase. The average D90 also increases, from roughly 7.4 μm to 9.6 μm.

The SiOx particle size and coating thickness move together through SoC. Both stay approximately level from 0% to 75% state of charge, then rise at 100%. Polaron is able to capture and quantify how these interactions are related directly from the SEM images.

These measurements describe electrode structure in 2D and compare different electrodes rather than tracking individual particles during charging. Polaron extends this analysis by generating statistical 3D reconstructions from the segmented SEM images. These reconstructed volumes are then used to calculate 3D metrics, such as pore tortuosity, and to estimate how the surrounding pore network affects transport.

Tortuosity links the reconstructed pore geometry to transport

Pore fraction describes the amount of space available to the electrolyte, but not the efficiency of the path through that space. Two electrodes can have the same porosity while one contains relatively direct, connected pores and the other contains narrow, convoluted or disconnected pathways. Tortuosity is used here to distinguish those cases.

Five 3D reconstructions were generated at each state of charge (totalling 25 cubes), each a cube 51.2 μm along each side. In every reconstruction the pores form a connected 3D network, and the tortuosity factor, , is calculated directly from that network. Tortuosity values for each volume (grouped by their respective SoC are displayed in Figure 7.  The mean through-plane pore tortuosity increases from 3.3 at 0% SoC to 5.0 at 25%, 7.4 at 50%, 16.1 at 75% and 16.4 at 100%.

Figure 7: Tortuosity through the pore phase on the 3D reconstructed volumes vs state of charge. Tortuosity values were obtained using Taufactor 2 on Polaron.

Referring back to Figure 3,  the pore fraction was shown to decrease to approximately 16% by 50% SoC and then plateaus through 100% SoC. The tortuosity factor does not follow this plateau. It continues to increase, indicating that the remaining pore network imposes a progressively greater transport penalty even though the pore fraction itself changes little. Pore fraction alone therefore cannot fully describe transport through the electrode: it quantifies the amount of pore space but not the connectivity or path lengths that determine how effectively ions can move through it. These changes become apparent only when the pore network is analysed in the reconstructed three-dimensional volumes.

Comparison to Bruggeman relationship

A classical Bruggeman relationship provides a useful reference:

Where Deff is the effective diffusivity, Dbulk is the unobstructed diffusion coefficient and is the porosity. Under the tortuosity convention above, 

this corresponds to

Using the mean 2D pore fractions as estimates of porosity gives Bruggeman tortuosity estimates of approximately 1.7-2.6.  The 3D reconstructed volumes give mean tortuosity factors of 3.3-16.4. A comparison between the Bruggeman estimates and the tortuosity values determined directly from the volume is presented in Figure 8.  This shows that the Bruggeman relationship underestimates the transport resistance of these 3D electrode structures, which is consistent with the known limitations of applying the Bruggeman approximation to electrode microstructures.

Figure 8: Polaron reconstructed tortuosity vs the Bruggeman estimate at various states of charge.

Conclusion

This blog shows how Polaron combines quantitative SEM analysis with statistical 3D reconstruction to compare Gr-SiOx electrodes across five states of charge, from 0% to 100%.

From the raw images, Polaron segmentation shows that porosity decreases substantially between 0% and 50% SoC, alongside an increase in the graphite fraction. Electrode thickness remains approximately constant through 75% SoC and increases by 12% at 100% SoC. SiOx particle size also rises between 75% and 100% SoC.

Polaron’s 3D reconstructions then show that tortuosity rises sharply between 50% and 75% SoC, where the mean 2D pore fraction is approximately stable, and then changes little through 100% SoC. Across the measured states of charge, tortuosity remains consistently higher than the Bruggeman estimate. Porosity volume fraction alone does not fully describe pore-phase transport; the three-dimensional morphology of the pore network has to be considered as well.

Taken together, Polaron links particle size, electrode thickness, phase fraction and pore transport using the same microscopy data. This enables rapid comparison of electrode formulations, calendering conditions and processing methods, helping to prioritise candidates for cell-level testing and reduce the number of build-and-tear-down iterations required. The analysis can also provide electrochemical models with SoC-dependent estimates of porosity and tortuosity – parameters that are often treated as fixed or simplified.

About Polaron

Polaron is making better materials possible with microstructure intelligence. We develop AI models that read microstructure from the images teams already collect, connecting how a material was made to how it performs. Engineers at leading materials manufacturers across the globe use Polaron to accelerate root cause analysis, improve quality and develop better materials. Polaron spun out of Imperial College London after nearly a decade of research in AI and materials science and has since raised over $8 million in funding.

Get the next teardown in your inbox

New teardowns, benchmarks and design data from BatteryDesign.net, free by email. Unsubscribe any time.

Leave a Comment